A transparent part has nowhere to hide a defect. A flow mark, a small bubble or a fine scratch on the mold surface that would be invisible on an opaque part is immediately seen on a clear one. Lighting diffusers, lenses, display windows and clear covers therefore demand extra care in both the mold and the process.

Transparent materials

Material Key property Watch out for Typical use
PMMA (acrylic) Highest light transmission, scratch and UV resistance Brittle; low impact strength Lenses, light guides, diffusers
PC (polycarbonate) Very high impact strength, heat resistance Absorbs moisture; poor drying causes silver streaks and bubbles; scratches easily Luminaire housings, protective covers
PS (crystal) Economical, easy to process Brittle, yellows under UV Packaging, disposables
SAN Chemical resistance, stiffness Limited impact strength Housewares, cosmetic packaging
Transparent ABS (MABS) Balance of toughness and clarity Lower transmission than PMMA and PC Housings and covers
PETG / copolyester Toughness, chemical resistance Low heat resistance Medical and food packaging

What matters in the mold

  • Steel selection: clean, stainless-type mold steels that can hold a mirror polish are preferred; the smallest inclusion shows up as a pit during polishing.
  • Polishing: cavity and core faces are brought to mirror quality in steps with diamond paste. Polishing time has to be added to the lead time.
  • Gate: the melt should enter calmly on a single front. Fan and film gates prevent jetting; where possible the gate is moved to a hidden edge.
  • Venting: trapped air shows as burns and haze on a clear part; vents are cut at the last points to fill.
  • Ejection: ejector marks must not fall on optical faces; ejection is done from the edge, by stripper plate or ejector frame.
  • Mold temperature: transparent materials want a hotter mold; even cooling reduces internal stress and optical distortion.

In part design

  • Keep wall thickness uniform. Thick sections cause voids and sink, both visible in a clear part.
  • Make thickness transitions gradual; abrupt changes leave flow marks.
  • Avoid sharp inside corners; PMMA and PS are very notch sensitive.
  • Do not put ribs or bosses behind an optical face; they read through to the front.
  • Polished faces need draft too; with too little draft the part scratches on ejection.
  • Agree early where the weld line will fall; on a clear part it cannot be hidden by texture.

In the process

  • Resin must be dried at the time and temperature given by its producer; moisture is the number one enemy of clear parts.
  • Screw and barrel must be clean; the smallest residue from a previous material appears as a black speck.
  • Regrind is limited or not used at all.
  • Parts are protected individually after ejection so they do not scratch.

The earliest decision is the cheapest

Gate location, weld lines and air traps can be seen before the mold is built with a mold flow analysis. For surface classes see our Surface Finishes Guide.

Request a Quote

Kalıp ve hassas parça işleriniz için üretim ortağınız

Kokil, plastik enjeksiyon ve alüminyum enjeksiyon kalıpları ile CNC talaşlı imalat tek atölyede. Teknik resminizi gönderin, birlikte değerlendirelim.

Bize Ulaşın
Kasım 16, 2026

Stainless Steel Grades in CNC Machining: 303, 304, 316, 420 and 17-4 PH

Devamını oku
Kasım 16, 2026

CNC İşlemede Paslanmaz Çelik Türleri: 303, 304, 316, 420 ve 17-4 PH

Devamını oku
Tüm haberler ve yazılar